! POLY OXIDATION @ 800C Pyrogenic Steam ! Target: 225 20 on single crystal silicon ! Filed : POLYREOX.R Tube: 1 Recipe: 00:10:00 D Push 800C Ar @ 9.0 l/m + O2 @ 0.2 l/m Push @ 10"/min 00:05:00 W Soak 800C Ar @ 5.0 l/m + O2 @ 0.2 l/m 00:35:00 W Wet 800C O2 @ 4.0 l/m + H2 @ 8.0 l/m 00:30:00 D Anneal 800C Ar @ 5.0 l/m 00:05:00 D Cool 800C Ar @ 5.0 l/m 00:20:00 D Pull 800C Ar @ 9.0 l/m Pull @ 5"/min